In a message dated 06/22/2000 6:16:34 PM Central Daylight Time,
[log in to unmask] writes:
> Ken - I suggest you consider using Sn62 solder to slow down the leaching of
> the Palladium-Silver termination. Do you have a barrier layer or is this
> just a single layer termination? If a single layer, you may only get one
> reflow cycle out of the termination before it dissolves into
> non-wettablility. Why don't you use a standard 3-layer termination?
>
> Ed Valentine
> Electronics Manufacturing Solutions
> 8612 Mourning Dove Road, Raleigh, NC 27615
> Phone: (919) 270-5145, Fax: (919) 847-9971
> Email: [log in to unmask]
> Website: http://www.ems-consulting.com
Hi Ken!
I agree with Ed. I ran across some thermistors that had palladium silver
terminations and used a 2% silver paste and the joints looked much better.
These components can't take touch-up though...you put a soldering iron to
them and "POOF" the terminations disappear! (least they did on the
thermistors I dealt with) Your QA will need to back off on how high the
fillets go up the terminations, they won't flow up as high like a tin/lead
termination does. It'll just look a little different like T.I. parts do with
the palladium plating. DON'T TOUCH THEM UP!
-Steve Gregory-
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|