The Black Nickel issue is a very low level defect (ppm), with big
ramifications when it is encountered. In absence of a good understanding of
how this occurs, it has become a "Catch all" for any solderability issues
associated with ENIG. Many defects that may have other explanations go un
investigated once they are labeled "Black Nickel".
The immersion gold step is a controlled corrosion reaction. Occasionally
this could go out of control and may create a "Black Ni" pad, under the
immergent Au. This gold will have a tendency to peel if tape tested,
depending on the degree of severity of the corrosion. The underlying Ni is
compromised and may not wet.
Some of the ways that this can occur are:
Uneven Ni deposit:
An uneven Cu surface (pitted, corroded etc)
Solder mask residues on the incoming Cu surface
Cu/tin intermetallics as above
Uneven catalyzation. Catalyst bath operated out of control.
Ni bath chemistry out of the specified operating range
Gold bath too aggressive:
Excessive dwell time in the Au bath
High Temperature (outside the control limits)
Au bath chemistry out of specified range.
Most board shops today are fully aware of this condition and are making sure
that their ENIG processes are running within the specified vendor
recommendations.
George Milad
Shipley
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|