Bruce,
DBC stands for Direct Bonded Copper. It's a process where you plate Cu on substrates and often used in for example hightemp amp applications.
Stellar Industries is one of many who make this.. http://www.stellarind.com/5metllz.html
Yes I know, the FET needs a very good thermal path and wire bond.
To solder the FET with Au/Sn requires high temperature, but if a substrate has combined ThickFilm (to which you mount components with Ag-epoxy) with DBC (to which you solder the FET) and want to replace the FET. That's a problem.
Our Ag-epoxy don't appreciate high temperatures and you can't avoid heating up the surrounding components, when trying to remove the FET, because of the the concept (TF & DBC).
From there, I see two ways. Either replace the epoxy or replace the solder to one kind where the surrounding temperature, when removing FET, won't harm the Ag-epoxy. So, a low(-er) temperature solder around 160-200degC would be nice.
Any ideas? Anyone?
__________________________________________________
Jan Merstrand
Microwave MCM, Design/Production Support
Ericsson Microwave Systems AB. Defence Manufacturing
Office address: Bergfotsgatan 2, SE-431 84 Mölndal
Phone: +46 31 747 0725, Fax: +46 31 747 3515
> -----Original Message-----
> From: Misner, Bruce [mailto:[log in to unmask]]
> Sent: den 30 mars 2000 16:11
> To: [log in to unmask]
> Subject: Re: [TN] Solder at lower temperature
>
>
> Jan,
>
> The FET requires 2 things: excellent thermal path and wire bonds. AuSn
> provides a thin interface with minimal voiding without flux
> (although N2
> enviornment or blanket is required). This is good for both
> requirements and
> hence has always been the material of choice in this
> situation, especially
> for high rel applications (I see you are a Defense
> contractor). It also has
> the added benefit of not leaching Au (because it already is
> 80% Au) and
> allows additional processing of other areas of the assembly
> at solder temps
> without reflowing the original interface. Unfortunately, I'm
> not familar
> with acronim "DBC" for substrate (European vs American?). If
> you can better
> define this material I might be able to make other suggestions for FET
> attach.
>
> One last note is that FETs can reach high delta T junction temp. This
> combined with the operating temp can bring the interface
> dangerously in the
> range of typical solder (SN63) reflow temps. Hope this helps.
>
> Bruce Misner
>
> > ----------
> > From: Jan Merstrand
> (EMW)[SMTP:[log in to unmask]]
> > Reply To: TechNet E-Mail Forum.;Jan Merstrand (EMW)
> > Sent: Thursday, March 30, 2000 4:11 AM
> > To: [log in to unmask]
> > Subject: [TN] Solder at lower temperature
> >
> > Hi guys and girls!!
> >
> > I have a question that I think many of you can answer.
> > Today we solder FET chips with Au/Sn solder onto a DBC
> substrate with Au
> > surface.
> > The soldering area of the FET is Chromium/Nickel/Silver.
> >
> > I want to replace the Au/Sn solder with "something else"..
> I don't want to
> > glue the chip to place, only solder.
> > The FET working temperature reaches up to 120degC.
> >
> > Any ideas on what kind of solder to use?
> > __________________________________________________
> > Jan Merstrand
> > Microwave MCM, Design/Production Support
> > Ericsson Microwave Systems AB. Defence Manufacturing
> > Office address: Bergfotsgatan 2, SE-431 84 Mölndal
> > Phone: +46 31 747 0725, Fax: +46 31 747 3515
> >
> > ##############################################################
> > TechNet Mail List provided as a free service by IPC using
> LISTSERV 1.8c
> > ##############################################################
> > To subscribe/unsubscribe, send a message to [log in to unmask] with
> > following text in
> > the body:
> > To subscribe: SUBSCRIBE TECHNET <your full name>
> > To unsubscribe: SIGNOFF TECHNET
> > ##############################################################
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> > additional
> > information.
> > If you need assistance - contact Keach Sasamori at [log in to unmask] or
> > 847-509-9700 ext.5315
> > ##############################################################
> >
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using
> LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask]
> with following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm)
> for additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
>
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|