Hi Steve,
My comment has nothing to do with Ag-containing solders, but with the effect
of Ag-plating on component leads. Immersion Ag may be thin enough not to give
you the necessary Ag concentration.
The experience I referred to goes back to about 1982. The industry found
out—and since forgot except for a few old-timers like me—what silver can do
to solder joints, when TI moved some of its PLCC production to Singapore.
There somebody decided to Ag-plate the leads. At the first unfortunate
recipient of this product, IBM-Austin, the PLCCs started to literally fall
off the PCBs when slight bending, such during fixturing for functional
testing, put even very small loads onto the solder joints. As a consequence
of this scary news (nobody knew about the Ag yet and compliant leads were
just invented and without history), 17 competing companies joined forces and
formed the IEEE Compliant Lead Task Force.
Silver, it turns out creates an even weaker intermetallic compound (IMC) with
tin than does gold. The necessary IMC concentration necessary for this effect
is about the same as for Au.
Because of legal problems (the 2 companies with the lowest PLCC fatigue lives
threatened to sue everybody involved in the IEEE CLTF), the results, except
for some preliminary data, were never published.
If you go back into the TechNet archives, you will find some problems related
to Ag (plating) being discussed.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 904-437-8747, Fax: 904-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|