Alain,
It sounds like a capacitor that had its termination over fired resuting in
excessive glass diffusion into the base ceramic, excessive thick nickel
plating, a combination of the two, improperly fired ceramic (overfired),
excessive solder and rapid cool down, perhaps even wave solder or hand
solder operations that were uncontrolled.
John Maxwell
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Alain Mathieu
Sent: Wednesday, January 26, 2000 11:45 AM
To: [log in to unmask]
Subject: [TN] Metallization problem on chip capacitors
Hi TechNetters.
We recently discovered a problem on chip capacitors: when examine carefully
with magnifying glass, we found a separation (Gap) between the endcap
(metallization) and the ceramic.
When capacitors were pried with tweezers, the whole ceramic part came off,
leaving both, complete endcap in the solder joints.
Removed caps were examined under microscope and all we could see was a
brownish deposit ( look like glue ) where the two endcaps were.
I think it is a part manufacturing problem. Am I right to think that or can
something else have cause the separation of the endcaps ?
Alain Mathieu
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|