Arnaud Grivon <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Arnaud Grivon <[log in to unmask]>
Date:
Wed, 21 Oct 2009 09:26:44 +0200
Content-Type:
text/plain
Parts/Attachments:
text/plain (77 lines)
Hello,

I am seconding Inge's comments : a too low or borderline Au thickness 
may be the cause of your problem. The first reflow may oxidize the 
underlying Ni layer and makes the topside wetting difficult. A too low 
Ni thickness is also a known source of soldering problems, but it 
doesn't fit well with your case as the first side is soldering well and 
the Ni thickness is usually consistent between the 2 PCB sides.
You will be able to state on the Ni thickness on cross-section, but you 
need XRF on bare boards for the Au thickness.
Regards,

A. Grivon

Hernefjord Ingemar a écrit :
> Bill,
>
> While the gurus are quarreling about black pad definition, I try to see if there is a logical alternative. You said that you soldered only ONE side, the backside. And the topside was NOT soldered, is that right? I remember we had a similar problem many, many years ago. What happened then was this: the Immersion Gold was nearly non-existent, and the underlying nickel plating was not the best either. So, when we mounted the topside, after having soldered the backside, and ran the boards through the oven, the solder melted, wetted on the Immersion Gold, but after the gold was consumed and the solder was expected to wet on the nickel, there was no proper wetting, so the solder withdraw, or with other word, dewetted. When the backside was soldered, the topside ENIG was degraded, i.e. the nickel was oxidized. There was nothing we could do about it, other than send back the boards. There were many tours before our board supplier got a proper process control.
>
> Inge
>
>  
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of [log in to unmask]
> Sent: onsdag 21 oktober 2009 01:21
> To: [log in to unmask]
> Subject: [TN] ENIG Issue
>
> Fellow TechNetters:  I ran into a problem and I am looking for more information.  We had some PCB made with ENIG for SMT applications.  We populated the backside, ran them through the convection oven, the solder fillets were fine.  Populated the first five (5) PCBs on the topside, ran them through the convection oven, and the solder fillets were quite bad, actually dewetted.  Could not even be touched up.  Tried two (2) more random PCBs and got the same results.  Never have run into this before but have been told it is NOT a unique problem.  Has anybody had this happen?  Have to tell our customer that they are not going to be getting their PCBs on time and would rather not look like the north end of a southbound mule.
>
>
>
> Thanks in advance for your assistance.
>
>
>
> Bill Black
>
> 1 631 667 9699   X13
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>   

-- 
Arnaud Grivon
Thales Corporate Services - EPM
18, Avenue du Maréchal Juin
Bât. C - Bureau C2-135
92366 MEUDON LA FORET Cedex
Tél : (+33) (0)1 70 28 23 88


"The information contained in this e-mail/fax and any attachments are the property of THALES and may be confidential. If you are not the intended recipient, please notify us immediately, send this message back to us and destroy it. You are hereby notified that any review, dissemination, distribution, copying or otherwise use of this e-mail/fax is strictly prohibited." 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2