Hi,
Since you say that the component is concave, there is a possibility that the urethane coating is collecting together due to this concavity. When the coating thickness increases, the chances of bubbling increase. There is always a possibility that the surface is not clean enough.....try the following
1. take a fine grit paper and if possible rub gently to try to roughen the surface to make the coating stick (this is especially useful for IC topside, where the surface is very smooth
2. spray a very fine mist of Xylene and wait for a couple of minutes before spraying (this worked wonders for me for a board that was dewetting like crazy)
Amol Kane
M.S (Industrial Eng.)
Process Engineer
Harvard Custom Manufacturing
941 Route 38 Owego, NY 13827
Phone: (607) 687-7669 x349
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Blair K. Hogg
Sent: Tuesday, January 24, 2006 10:40 AM
To: [log in to unmask]
Subject: Re: [TN] Conforma Coat (Urethane) & bubbles
This is just a guess, and nothing more, but could there possibly be outgassing from something in the component? I'm pretty skeptical of this, since any outgassing should have already occurred, but may be happening due to the rise in temperature?
>>> [log in to unmask] 01/24/06 10:25AM >>>
We've got a problem here, where we're hand spraying a urethane conformal
coat on over a rectangular inductor.
The inductor body is a plastic tube, with potting to fill.
The top is not always flat (sometimes concave).
The problem is that bubbles appear in the conformal coat on the potted
surface, sometimes right after bake and sometimes days after.
Any ideas on what the root cause is and how to prevent the bubbles?
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
*******************************************************************
This email and any files transmitted with it are confidential and
intended solely for the use of the individual or entity to whom they
are addressed. If you have received this email in error please notify
the system manager.
This footnote also confirms that this email message has been swept
for the presence of computer viruses.
www.hubbell.com - Hubbell Incorporated
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|