Hi Eric! Just a word of clarification - yes it is true that you do not need
to make an intermetallic to create a reliable joint provided the two
elements you are working with form a solid solution couple. However, the
action of creating a solder joint is not the joining of tin and lead but
the joining of a tin/lead alloy with copper - the formation of a copper/tin
intermetallic is critical for a reliable solder connection. Hanson's book
is a great reference - you may also want to take a look at the new edition
of the American Welding Society (AWS) handbook (3rd edition) for inclusion
in your library (ISBN 0-87171-618-6). Dr. Paul Vianco and the AWS committee
did an wonderful job of updating the handbook with new material (lots of
phase diagrams, references, etc.).
Dave Hillman
Rockwell Collins
[log in to unmask]
Eric Dawson <[log in to unmask]>@ipc.org> on 10/23/2001 02:14:04 AM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: Re: [TN] tin on iron and solder on iron
Guy,
I'm now curious. Why little old ladies? what were they making with these
wired nails? and why were you watching them?
I hope I don't regret asking these questions, we know what happened to the
curious cat!
On a more serious note, and to address the original question,
intermetallics
will form between two metals when that is the stable reaction. See Hanson's
'Constitution of Binary Alloys.' This is a very good standard reference
work, though probably out of print by now. It is known that the Romans
soldered lead piping for their plumbing systems (plumbum-lead) and this
would not have formed any intermetallic even though good joints were made.
In this case the tin and lead form a solid solution which is the stable
product of the two metals involved. Therefore, it is not strictly correct
to
say that an intermetallic is a requirement for a good soldered joint,
rather, that the intermetallic is a product of a good soldered joint
between
copper and tin or iron and tin.
The flux is there to remove oxides and allow the solder and the base metal
to come into intimate contact and to aid heat transfer.
Regards
Eric Dawson
> -----Original Message-----
> From: Guy Ramsey [SMTP:[log in to unmask]]
> Sent: Monday, October 22, 2001 7:51 PM
> To: [log in to unmask]
> Subject: Re: [TN] tin on iron and solder on iron
>
> It must be flux strength. I have watched little old ladies solder wires
to
> nails. They were using zinc chloride. Destroyed the solder iron tips but
> did
> what they wanted.
>
> We also made some custom tips for Pace solder pens. They were stainless,
> we
> solder plated them too. They did not last as long nor work as good as the
> store bought ones but they were less expensive. We did not measure the
tip
> temperature offset . . . oh yeah you were only asking about soldering
iron
> .
> . . ramble on.
>
>
>
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]]On Behalf Of Bev Christian
> > Sent: Monday, October 22, 2001 2:34 PM
> > To: [log in to unmask]
> > Subject: Re: [TN] tin on iron and solder on iron
> >
> >
> > OK, let me try saying this a different way:
> > it "seems" that the canning industry has an easy time putting tin on
can
> > steel. Why do I have trouble getting solder to stick to a properly
> > preheated 100% iron surface? Is it just a matter of flux strength? Or
> > something else?
> >
> > Bev Christian
> > Research in Motion
> >
> > -----Original Message-----
> > From: Mel Parrish [mailto:[log in to unmask]]
> > Sent: October 22, 2001 4:17 PM
> > To: [log in to unmask]
> > Subject: Re: [TN] tin on iron and solder on iron
> >
> >
> > Dr Bev,
> > Not sure what your question is but for discussion. Many of the common
> > component lead frames contain significant amounts of iron which
> > is plated to
> > enhance solderability, limit corrosion, etc.. Seems that there should
> be
> > some metallurgists out there that can lead us to understanding the
> > solubility characteristics but my text books discuss FeSn intermetalics
> > although the rate is slower that that of tin gold or tin copper.
> > Also seems
> > to me that the Nickel content is important to the solder interface.
> >
> > Mel Parrish
> > Soldering Technology International
> > 102 Tribble Drive
> > Madison, AL 35758
> > 256 705 5530
> > 256 705 5538 Fax
> > [log in to unmask]
> >
> > -----Original Message-----
> > From: TechNet [mailto:[log in to unmask]]On Behalf Of Bev Christian
> > Sent: Friday, October 19, 2001 2:01 PM
> > To: [log in to unmask]
> > Subject: [TN] tin on iron and solder on iron
> >
> >
> > OK, here is a general question for all you met guys. But I am not sure
> I
> > can explain it well enough to be understood!
> >
> > We all know that tin can be put on iron or we wouldn't have "tin" cans.
> I
> > also know it is difficult to put solder on iron. So my question
> > is this: if
> > one has a tinned iron surface and it is put into molten solder
> > the tin will
> > be dissolved into the molten solder. I presume when the piece of iron
> is
> > withdrawn from the pot, solder will be well adhered to the iron. Is
> this
> > because there is a solderable tin/iron intermetallic? What is the main
> > difference between the tin can process and putting solder directly on
> iron
> > that makes one easy to do and the other difficult? This may be a
"first
> > grade" met question, but I don't know the answer. Thanks.
> >
> > Bev Christian
> >
> > ------------------------------------------------------------------
> > ----------
> > -----
> > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt delivery of Technet send the following message: SET
> > Technet NOMAIL
> > Search previous postings at: www.ipc.org > On-Line Resources &
Databases
> >
> > E-mail Archives
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> > additional
> > information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
> > ext.5315
> > ------------------------------------------------------------------
> > ----------
> > -----
> >
> > ------------------------------------------------------------------
> > ----------
> > -----
> > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt delivery of Technet send the following message: SET
> > Technet NOMAIL
> > Search previous postings at: www.ipc.org > On-Line Resources &
Databases
> >
> > E-mail Archives
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> > additional
> > information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
> > ext.5315
> > ------------------------------------------------------------------
> > ----------
> > -----
> >
> > ------------------------------------------------------------------
> > ---------------
> > Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> > To unsubscribe, send a message to [log in to unmask] with following text
> in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt delivery of Technet send the following
> > message: SET Technet NOMAIL
> > Search previous postings at: www.ipc.org > On-Line Resources &
> > Databases > E-mail Archives
> > Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> > additional
> > information, or contact Keach Sasamori at [log in to unmask] or
> > 847-509-9700 ext.5315
> > ------------------------------------------------------------------
> > ---------------
> >
>
>
--------------------------------------------------------------------------
> -------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases
>
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
>
--------------------------------------------------------------------------
> -------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|