Another thought, is your assay OK?
Rex Waygood
Technical Manager
PartnerTech Poole Ltd
Benson Road
Poole
Dorset BH17 0RY
United Kingdom
Tel: +44 (0)1202 674333
Fax: +44 (0)1202 678028
DDI: +44 (0)1202 338222
Mob: +44 (0)7887 997403
[log in to unmask]
www.PartnerTech.co.uk
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: 29 November 2007 15:19
To: [log in to unmask]
Subject: Re: [TN] SN100C process
Mike,
Thanks for the insight. What worries me is that 540F is actually 280C. I didn't go there yet, but I am at 274C (525F) and still see the solder freezing at the corners of the pot. Although this must be a machine issue, did not get much help from the manufacturer.
I've got your point regarding VOC free fluxes.
Thanks,
Ioan
-----Message d'origine-----
De : Mike Fenner [mailto:[log in to unmask]] Envoyé : 29 novembre 2007 09:47 À : 'TechNet E-Mail Forum'; Ioan Tempea Objet : RE: [TN] SN100C process
While we wait for Ronnie......
540F is about 250something C, that's about in the 'normal' range. Don't forget the SN100C is a tin/copper not a SAC and so has a higher MP/operating range.
For LF wave soldering you probably need to have a little higher solids than for leaded, and some VOC formulations are definitely more suited to lead free than IPA based materials. This is all down to the properties of high SN content of lead free alloys and their associated temperatures as a whole rather than specific differences between them.
You should be able to solder satisfactorily without nitrogen as a soldering aid, but do have nitrogen as a dross limiter.
Specific process parameters will depend on your specific alloy ,machine, flux and board type. You will probably be better to have those conversations individually off line or get ideas from other user experiences.
Overall there is no intrinsic reason why you should not be able to wave solder lead free with very low defect levels, board/design/components are still the ultimate limiting factors in this process.
Regards
Mike Fenner
Indium Corporation
T: + 44 1908 580 400
M: + 44 7810 526 317
F: + 44 1908 580 411
E: [log in to unmask]
W: www.indium.com
Pb-free: www.Pb-Free.com
---------------------
Indium Corporation
Incorporated in New York, USA
Registered office: (Not for correspondence)
77-97 Harpur Street, Bedford , UK
Registered number: fc16473
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: Wednesday, November 28, 2007 3:55 PM
To: [log in to unmask]
Subject: [TN] SN100C process
Dear Technos,
I have moved to this new company and here we're running SN100C in wave, as
opposed to the SAC305 I used to have before. So I have to start all over
defining the baseline process parameters.
Besides frequent shorts and solder not going all the way to the top, we have
an issue with solder freezing at the corners of the solder pot. To overcome
this "chilly" issue, we were suggested to run the pot at 540F!
So I would like to know where you are with the SN100C:
* What pot temperature
* What conveyor speed range
* What flux (special formulation for the alloy or regular,
solids content, water or alcohol based, etc)
* Nitrogen or not
* Other particular points of interest
Of course an insight regarding the attainable defect free yields would also
be appreciated.
Thank you,
Ioan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited.
Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after is was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***"
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
-------------------------------------------------------------------------------
The information contained within this e-mail and any attachments contained therein may be confidential and/or legally privileged and is for the use of the intended recipient only. If you are not the intended recipient please delete it from your system and notify the sender by return e-mail. The content of this e-mail may not be copied or disclosed to any third parties without prior permission from the sender.
E-mail is susceptible to data corruption, interception, tampering and viruses. We do not accept any liability for any such incidents or any consequences thereof.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|