Mike,
You are somewhat correct, but this prep/tin method gave us
better results than just trying to solder the parts into the board with
a straight RMA. And as we could not use a OA/IA flux on the entire
assembly, it was our best option to improve the overall solderability of
the parts.
Mike
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mike Fenner
Sent: Tuesday, August 24, 2004 11:09 AM
To: [log in to unmask]
Subject: Re: [TN] Soldering Nickel Leads
True, but the original question was to only use an RMA flux....
Prepping with the Kester or similar products then removing them and then
using an RMA would put the same chemical activity or more as simply
using a water washable IA flux and cleaning onto the assembly. So
although the final soldering would be done with an RMA, the difference
is mostly semantics (prep chemical versus flux). Chemically there would
be little difference to using an IA flux only.
Regards
Mike
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mike McMonagle
Sent: Tuesday, August 24, 2004 3:25 PM
To: [log in to unmask]
Subject: Re: [TN] Soldering Nickel Leads
Kester makes a product called Nickel Nu for prepping nickel or Kovar
leads before soldering:
http://www.kester.com/en-us/products/prodcat_detail.aspx?pid=104
You can request a sample if you only have a few parts to do, or order a
gallon and you'll be set for a loooonnngg time. Or you can roll your own
if you don't want to buy it, it's basically hydrochloric acid and copper
dichloride diluted in DI water. Take all prudent precautions when
handling, it can be very nasty stuff. We have used it (or the homebrew
version) to prep nickel leads, then immediately rinsed with DI followed
by alcohol rinse. We then tinned the leads with the solder alloy that
the parts would ultimately be soldered with to protect them until that
point.
Mike
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mike Fenner
Sent: Tuesday, August 24, 2004 2:23 AM
To: [log in to unmask]
Subject: Re: [TN] Soldering Nickel Leads
Possibly you can get acceptable results by mechanically abrading the
lead, (there are special tweezers with abrasive pads, or you could even
use very fine grit "wet and dry" ) followed by as high a solids content
RMA as you can find. The high solids will increase the flux persistence
and therefore working time before displacement by the solder on dipping.
Regards
Mike Fenner
Indium Corporation
T: + 44 1908 580 400
M: + 44 7810 526 317
F: + 44 1908 580 411
E: [log in to unmask]
W: www.indium.com
Pb-free: www.Pb-Free.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Eric Kalgren
Sent: Tuesday, August 17, 2004 9:04 PM
To: [log in to unmask]
Subject: [TN] Soldering Nickel Leads
Hey all,
I have a minor problem with a component in house. The component leads
are 19 AWG nickel and I need to connect to them using 20AWG copper wire.
I looked in the archives for previous discussions on this topics and
came away with the impression that OA flux is required. My question is:
Can I solder these parts without having to go out and get some OA flux?
We use RMA and I'm reluctant to bring in a different flux and have it
used rather than the RMA. Can one mechanically prep the leads, then
flux with RMA, then dunk in the solder pot?
:::::::::::::::::::::::::::
This email, its content and any files transmitted with it are intended
solely for the addressee(s) and may be legally privileged and/or
confidential. If you are not the intended recipient please delete and
contact the sender by return and delete the material from any computer.
Any review, retransmission, dissemination or other use of, or taking of
any action in reliance upon, this information by persons or entities
other than the intended recipient is prohibited.
Messages sent via this medium may be subject to delays, non-delivery and
unauthorized alteration. This email has been prepared using information
believed by the author to be reliable and accurate, but Indium
Corporation makes no warranty as to accuracy or completeness. In
particular, Indium Corporation does not accept responsibility for
changes made to this email after it was sent. Any opinions or
recommendations expressed herein are solely those of the author. They
may be subject to change without notice.
:::::::::::::::::::::::::::
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|