Good point! I would suggest masking the upper via pads only, but
certainly not tenting them. That way, the solder will stop rising over
the top.
Brian
Dave Chapman wrote:
> ok, so today I had 10 boards with vias under the BGA and solder came up from
> wave solder machine and caused 4 shorts. Should the vias have been masked
> closed from the bottom? Should the metal ring at the top of the via
> (topside) have LPI over it so solder wont stick to it even if it does come
> up through the via hole? Should the bottom via ring have LPI over it so
> solder wont stick to it?
> Forget about process changes we will make those as far as speed and heat at
> wavesolder machine. What should I close if anything to stop the solder from
> getting up under the BGA's
> Dave C.
>
> -----Original Message-----
> From: Franklin D Asbell [mailto:[log in to unmask]]
> Sent: Friday, October 24, 2003 3:12 PM
> To: [log in to unmask]
> Subject: Re: [TN] Cleaning of via holes under components
>
>
> Curious, plugging with "solder" from only one side...what process is used
> for this??? Do you mean solder mask???
>
> Franklin
>
>
> ----- Original Message -----
> From: "David Douthit" <[log in to unmask]>
> To: <[log in to unmask]>
> Sent: Friday, October 24, 2003 1:21 PM
> Subject: Re: [TN] Cleaning of via holes under components
>
>
>
>>Brian,
>>
>>Well said (again!!)
>>
>>David A. Douthit
>>Manager
>>LoCan LLC
>>
>>Brian Ellis wrote:
>>
>>
>>>I'm a proponent of plugging -- with solder! Not only does it stop the
>>>contamination problem, but it is electrically and thermally desirable,
>>>as well. However, it should be done from only one side unless you like
>>>to see miniature Krakatoas.
>>>
>>>Brian
>>>
>>>Paul Baine wrote:
>>>
>>>>Hello,
>>>>
>>>>One of our Design Engineers is designing a surface mount PCB
>>>>assembly and would prefer not to have the via holes solder mask
>>>>tented. However, he is concerned that, if he does not call up
>>>>solder mask tenting on his bare PCB drawing, foreign matter could
>>>>find its way into a via hole and, if a component (e.g. an IC) was
>>>>mounted over the via hole, the foreign matter might not be removed
>>>>during the cleaning process.
>>>>
>>>>Has anyone had experience with this situation? I would appreciate
>>>>any help you could give me.
>>>>
>>>>Thanks very much in advance.
>>>>
>>>>Paul Baine
>>>>Q.A. Manager
>>>>C-Tech Ltd.
>>>>Cornwall, Ontario, Canada
>>>>
>>>>---------------------------------------------------
>>>>Technet Mail List provided as a service by IPC using LISTSERV 1.8e
>>>>To unsubscribe, send a message to [log in to unmask] with following text
>>>
> in
>
>>>>the BODY (NOT the subject field): SIGNOFF Technet
>>>>To temporarily halt or (re-start) delivery of Technet send e-mail to
>>>
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>
>>>>To receive ONE mailing per day of all the posts: send e-mail to
>>>
> [log in to unmask]: SET Technet Digest
>
>>>>Search the archives of previous posts at:
>>>
> http://listserv.ipc.org/archives
>
>>>>Please visit IPC web site
>>>
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information,
> or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
>
>>>>-----------------------------------------------------
>>>>
>>>>
>>>
>>>---------------------------------------------------
>>>Technet Mail List provided as a service by IPC using LISTSERV 1.8e
>>>To unsubscribe, send a message to [log in to unmask] with following text
>>
> in
>
>>>the BODY (NOT the subject field): SIGNOFF Technet
>>>To temporarily halt or (re-start) delivery of Technet send e-mail to
>>
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>
>>>To receive ONE mailing per day of all the posts: send e-mail to
>>
> [log in to unmask]: SET Technet Digest
>
>>>Search the archives of previous posts at:
>>
> http://listserv.ipc.org/archives
>
>>>Please visit IPC web site
>>
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information,
> or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
>
>>>-----------------------------------------------------
>>
>>---------------------------------------------------
>>Technet Mail List provided as a service by IPC using LISTSERV 1.8e
>>To unsubscribe, send a message to [log in to unmask] with following text in
>>the BODY (NOT the subject field): SIGNOFF Technet
>>To temporarily halt or (re-start) delivery of Technet send e-mail to
>
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>
>>To receive ONE mailing per day of all the posts: send e-mail to
>
> [log in to unmask]: SET Technet Digest
>
>>Search the archives of previous posts at: http://listserv.ipc.org/archives
>>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
>
>>-----------------------------------------------------
>>
>>
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
> -----------------------------------------------------
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|