In a past life, we had an issue that manifested in a similar manner.
It was random deposition of silver/black spherical shaped contaminate
on ENIG and turned out to be...solder paste contamination on the
surface from support system in printer. They were very uniform in size
because the paste sphere is pretty darn uniform.
I suppose SEM/EDX could tell you what it is, but, if you don't own,
that's spendy. Have you tried XRF to see if it's got a solder-like
profile?
It's strange that they tape the plane and it still comes on...wonder
if they have a poor cleaning process for misprints and just tape over
it. I may have missed, but how random does this manifest (eg same spot
on every CCA, same spot on some CCAs, different locations on some
CCAs, etc)
Sent from my iPhone
> On Jul 29, 2014, at 3:50 PM, "Stadem, Richard D." <[log in to unmask]> wrote:
>
> I don't think they are solder splashes, because I blew the picture way up and noted the same thing Dave pointed out: they are too uniform to be random solder splashes, and the center black dot is always smack dab in the center, and when you greatly magnify the picture it appears that these are actually open holes in the gold plating, ie, the gold plating appears to curve down into the silver area that is perfectly centered around a small black dot in each location.
> Have these been examined under a good microscope, like 40x or better?
> You might want to sacrifice a single CCA and have the "splashes" microsectioned. It may tell you quite a lot.
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan TEMPEA
> Sent: Tuesday, July 29, 2014 2:27 PM
> To: [log in to unmask]
> Subject: Re: [TN] Trying to figure out possible mechanism for contamination
>
> Hi John,
>
> These are definitely solder splashes coming most likely from printing. If the assembler is covering the gold areas, you'll need to find out if they apply the Kapton prior to printing. Judging by the 0603 (or 0402?) caps and the miniBGA in the neighborhood, something tells me they would not want the Kapton there during printing, as it pushes the stencil up, increasing the paste volume with all the goodies that this can generate (shorts, tombstones, etc.).
> To make it more complicated, those tiny solder balls might even come from the table where taping is done. If the PCB is laid face down for some reason, it would gather no matter what. I know this situation, I've faced it many, many times and it's very hard to completely get rid of those splashes.
>
> One question: why would you want spotless gold on that large of a trace? If it's for grounding, as long as the splashes don't bulge up and hinder contact, there's plenty of Au surface to make a very good ground. Otherwise said, if you don't know for sure that small splashes like this affect form, fit or function, it would be a lot easier to live with them than trying to eliminate them. Of course, I'm talking about a reasonable amount of splashes, comparable to what shows in your photo.
> I guess at L3 you are doing intensive qualification of hardware and it would be easier to prove these splashes are benign than create massive rework.
>
> Regards,
>
> Ioan Tempea, P. Eng.
> Manufacturing Engineer
> Satellite Systems
> MDA
>
> This e-mail, and any attachments, are intended solely for the use of the intended recipient(s) and may contain legally privileged, proprietary and/or confidential information. Any use, disclosure, dissemination, distribution or copying of this e-mail and any attachments for any purposes that have not been specifically authorized by the sender is strictly prohibited. If you are not the intended recipient, please immediately notify the sender by reply e-mail and permanently delete all copies and attachments.
>
>
> -----Message d'origine-----
> De : TechNet [mailto:[log in to unmask]] De la part de John Foster Envoyé : Tuesday, July 29, 2014 12:13 PM À : [log in to unmask] Objet : [TN] Trying to figure out possible mechanism for contamination
>
> We have been seeing a problem recently on several different CCA'S that we are having assembled.
> The boards are ENIG with plug and plate. The assembly shop is assuring us that these gold areas are being Protected during the entire assembly process with kapton tape.
> I was thinking it was flux splatter since the areas are always almost perfectly circular.
> The locations are very random and range from nothing to what is in the picture.
> Is there any other mechanism that might be causing this? On our next run I am going to go to the shop To witness the taping. But I was curious if maybe it's some other cause.
> Mr. Gregory was kind enough to post a picture.
> http://stevezeva.homestead.com/spots.jpg
>
> Any thoughts would be appreciated
> Thank You
> John Foster
> L3 Communicatons
>
> Confidentiality Notice: The information contained in this message is intended only for the use of the addressee, and may be confidential and/or privileged. If the reader of this message is not the intended recipient, or the employee or agent responsible to deliver it to the intended recipient, you are hereby notified that any dissemination, distribution of copying of this communication is strictly prohibited. if you have received this communication in error, please notify the sender immediately.
>
> Warning: This document may contain technical data within the definition of the International Traffic in Arms Regulation (ITAR) and is subject to the export control laws of the U.S. Government. Transfer of this data by any means to a foreign person, whether in the United States or abroad, without an export license or other approval from the U.S. Department of State, is strictly prohibited
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|