John,
Would like to add this. Oftenly, the Ni under Au is rather bright and we
have seen rather frequently, that the nickel plating contains lots of
organics, like brighteners, grain enhancement agents, P-enriched voids
and other chemical stuff. Those ingredients slow down the solder wetting
process and many a time also cause lots of outgassing = voids.
Outgassing of Hydrogen seems worst. We have experimented with soldering
on matte nickel,
And the results have been amazing. Do you know if any bath makers are
offering such baths today for PWB?
Secondly, those working with solder wetting or glue wetting talk about
'time to obtain maximum wetting'. That the solder has flown out and
looks nice is not a proof that you have obtained the optimal IMC layers.
I have a very good article about soldering on Au/Ni, will see if I can
send that to Steve. May have to wait until I can send it from job
server, home modem to slow.
Inge
-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För John Maxwell
Skickat: den 29 oktober 2005 00:39
Till: [log in to unmask]
Ämne: Re: [TN] LEAD FREE PART IN SNPB PROCESS
David,
Salt or sugar for that matter in water is a solid to liquid diffusion
process. It like all diffusion processes is affected by time,
temperature and quantity of materials in the diffusion source. Soldering
is nothing more than liquid to solid diffusion with tin being the main
diffusion species into a base metal, typically copper or nickel. Before
this diffusion takes place, surface coating being solder (most common in
past), tin (probably most common in future), gold (i.e. an ENIG surface)
and PdAu over nickel on some semi lead frames must be dissolved. Then we
have solder joint formation. But if we just solder to the surface finish
we have not achieved tin diffusion into the base metal and that
diffusion results is solid crystalline structures called intermetallic
layers creating the solid bond between solder and component lead or pad
surface..
Also I have observed in the past if a reflow process is marginal then we
see ENIG "brittle fractures" and what has happened is the the gold has
not been completely dissolved restricting tin diffusion into the nickel
layer and there is soldering to the finish. There are two stable tin
gold eutectic alloys than can form and freeze out during solder joint
formation. One alloy is 80/20 Au/Sn with a eutectic temperature of 280C.
The other is Au/Sn 20/80 and has an eutectic temp of 240C. These frozen
zones are readily dissolved into the solder but if the time and temp are
not adequate the there are solder joint fractures in these zones. The
resulting fractured surface can be very smooth and frustrating. In the
last couple of year there was an excellent paper by some lads from
Taiwan who were able to capture solder joints with these zones frozen
and had some excellent photo in their paper. I believe it is available
thru the SMTA web site if one is a member.
John Maxwell
David Tremmel wrote:
> Hello,
>
> When someone equated soldering to that of salt dissoving in water, it
> threw
> me for a loop. Now I am wondering if someone willing to explain how
an
> inter-metallic bond is formed when one of the metals (Ni, in the
example
> below) is not in a liquid state?
>
>
> Thank you in advance,
>
> David
>
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|