Grant,
Unfortunately, without seeing the board or pictures of the problem I
can only give some general comments:
a) Differences in colour may be down to thickness variations in
the soldermask coating. Areas around vias or edges of high plated tracks may
appear lighter than the bulk.
b) Lightening of soldermask may also be due to moisture
absorption, sometimes seen after HASL or any other hot, wet post-processing
(ENIG for example). You may find that baking the board at 140°C - 150°C
(284°F - 302°F) for ~20 min will remove this effect.
As you also comment on a different finish (matte for light areas, glossy for
dark) I suspect your problem might be more related to (a) above, because you
are also seeing 'artwork marking' from the UV exposure process. You might
see this if you have a thicker ink deposit that has not been fully dried
prior to exposure.
I can't comment on possible effects on conformal coat, although I would
suspect that if the colour differences are due to moisture absorption you'll
want to get that out before considering overcoating.
Cheers,
David Albin
Coates Circuit Products
-----Original Message-----
From: Grant Emandien [mailto:[log in to unmask]]
Sent: 19 March 2002 09:36
To: [log in to unmask]
Subject: [TN] Soldermask color
Hi,
We have received PCBs with solder mask exhibiting color variarion i.e. light
and darker hues on the same PCB. The color differences are more prevalent
around vias but also evident on other areas. The light hue has a more matt
finish while the darker hue exhibits a sheen, almost an oily appearance but
is not easily removed.
Any comments on what it may be and possible effects (for conformal coating)?
TIA
Grant
**********************************************************************
Notice:
This email transmission contains confidential information which is the
property of the sender. The information is intended only for the use of the
addressee. If you are not the intended recipient, you are hereby notified
that any disclosure, copying or distribution of the contents of this e-mail
transmission, or the taking of any action in reliance thereon or pursuant
thereto, is strictly prohibited. Should you have received this email in
error, please immediately notify us by telephone to arrange for return of
the documentation comprising this transmission. In no event will Tellumat
(Pty) Ltd or the sender of this email be liable to any party for any direct,
indirect, special or other consequential damages for any use of this email,
or on any other hyper linked website, including, without limitation, any
lost profits, business interruption, loss of programs or other data on your
information handling system or otherwise, even if we are expressly advised
of the possibility of!
such damages.
**********************************************************************
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|