Edwin,
Standard FR-4 assembly practices apply to GETEK. It will hold up better in your soldering processes
than standard FR-4. GETEK has a higher glass transition temperature (Tg=175-185, DMA) than standard
FR-4 and close to but not as high as BT (ranges 170 - 215C depending on the grade). The CTE of GETEK
and BT are about the same (GETEK ~13ppm/C, BT 13-15 length, 15-17 cross).
You can get additional material properties from GE Electomaterials in Coshocton, Ohio at (740)
622-5310.
> ----------
> From: Edwin Maximo[SMTP:[log in to unmask]]
> Reply To: TechNet E-Mail Forum.;Edwin Maximo
> Sent: Thursday, January 07, 1999 5:23 AM
> To: [log in to unmask]
> Subject: [TN] Getek board
>
> Hi there,
>
> We will be conducting an evaluation on Getek and BT boards for one of
> our customers. This will be the first time for us to assemble
> components on a GEtek board, is there anyone out there who has
> experience or had a knowledge about Getek boards. What considerations
> should we have to look at e.g. profile for reflow, are there any
> difference between a BT board and a Getek board?
> Any information you could render will be appreciated.
>
> Regards,
> Edwin Maximo
> Value Engineer
> Electronic Assemblies Inc.
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional
> information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
> ################################################################
>
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|