According to the IPC Expo Paper in '99,
"Meeting Fine Pitch Assembly Needs with a Solderable Tin
Finish", by David Ormerod, The FST finish passed the
Siemens (Whisker Test) DIN41640 - 56 days @55'C/20%RH
(also long study tests of 35-45'C@85-93%RH). No Whiskers
were found.
Groovy
-----Original Message-----
From: Jerry Cupples [mailto:[log in to unmask]]
Sent: Friday, September 03, 1999 1:47 PM
To: [log in to unmask]
Subject: Re: [TN] Whiskers Problem on Leadframes
Stephané Menard asked:
>I have a question regarding the well known problem of whiskers generation
on
>leadframes.
>
>With the concept of lead free deposit and the investigation of several
>alternatives (Sn-Bi, Sn-Ag, Pure Tin, etc..) to Tin-Lead, we need to
study
>the risk of generation of whiskers with those substitutes.
>It is generally agreed that Tin alloys (even at low percentage in the other
>metal) are not prone to this problem whereas pure Tin deposits are.
>
>However, does anybody have a recognized method (electrochemical, physical,
>etc...) which could help in predicting the apparition, or not, of this
>problem (besides the standard aging test which sometimes can be quite
>doubtful !) ?
>
>I am looking forward to your answers and comments.
Michael Carano offered an interesting reply which concurs with my
experience, and also:
There is a method in which the electroplated coating is applied to thin
coupons which may be measured post plating for mechanical strain.
The concept is that whisker growth rate is a function of stress resulting
from the exact manner of the coating growth. Plating electrochemistry which
imparts less stress is also known to be more stable in regard to whiskers.
Sorry, I don't remember the source of these coupons, but check Metal
Finishing magazine (they used to have a website).
Plating coupons which have right angle minimum radius bends in a dry
cabinet at 120-150 degrees C will accelerate the formation of whiskers
visible with 10X magnification into the range of a few days. They seem to
form first on the outer bend radii.
regards,
Jerry Cupples
Interphase Corporation
Dallas, TX USA
http://www.iphase.com
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|