It is not at different temeperatures, nor at TC, but it is a vibration test.
Sincerly
Michael Jeremias,
-----Ursprüngliche Nachricht-----
Von: Joyce Koo [mailto:[log in to unmask]]
Gesendet: Freitag, 19. Dezember 2008 22:15
An: [log in to unmask]; Jeremias, Michael
Betreff: Re: [TN] AW: [TN] vibration testing of tin-lead and lead-free solder joints
Is it at two commercial temp extreme or high rel temp extreme?
--------------------------
Sent using BlackBerry
----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Fri Dec 19 13:03:08 2008
Subject: [TN] AW: [TN] vibration testing of tin-lead and lead-free solder joints
Unfortunately it is not allowed to copy it, but You can buy it at IEEE
Mit freundlichem Gruß
Michael Jeremias,
OPP41
Tel: 5533
-----Ursprüngliche Nachricht-----
Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Paul Edwards
Gesendet: Freitag, 19. Dezember 2008 18:32
An: [log in to unmask]
Betreff: Re: [TN] vibration testing of tin-lead and lead-free solder joints
Michael,
Is there a posting of this paper somewhere?
Paul
Paul Edwards
Surface Art Engineering
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Jeremias, Michael
Sent: Friday, December 19, 2008 3:20 AM
To: [log in to unmask]
Subject: [TN] AW: [TN] vibration testing of tin-lead and lead-free solder joints
Hi folks,
with this issue we have a fling or a big issue. This is what I knew up to now, supported by other papers. Thank You very much.
On the other hand there is existing a paper which tells exactly the opposite:
"Vibration Testing and Analysis of Ball grid Array Package Solder Joints" from Shaw Fong Wong e.a. Intel Technology 1-4244-0984-5/07/ 2007 IEEE
It says in the conclusion:
The comparison of SnAgCu and SnPb fatigue curves clearly indicated the better performance of SAC solder system under high cycle fatigue test.
I had not the time up to now to compare all boundary conditions, but in the paper of INTEL are Weibull curves drawn, which show that for cycles > 10**5 SAC survives SnPb. Vibration tests from about one hour ore more have more than 10**5 cycles..
This paper is already quoted in other papers and You can imagine that there is temporary a big uncertainity in the lead free society.
I would be happy if we can discuss about the big differences in the boundary conditions of these two worlds.
I started already comparing them, but I am interested in Your opinions. Is it the different annealing history or what?
Sincerely
Michael Jeremias
Industrial Engineering (OPPI41)
Electronics Production
((( Defence Electronics
EADS Deutschland GmbH
89077 Ulm
Tel.: +49 (0) 7 31.3 92-5533
Fax: +49 (0) 7 31.3 92-73 15
E-Fax: +49 (0) 7 31.3 92-20 5533
P Before printing, think about the environment !
-----Ursprüngliche Nachricht-----
Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Joe Fjelstad
Gesendet: Montag, 8. Dezember 2008 21:45
An: [log in to unmask]
Betreff: [TN] vibration testing of tin-lead and lead-free solder joints
Greetings folks
Found this on the wires today... (Cut it earlier out but lost the link but I am sure I am not the only one who read it. However I can go dig it up if there is interest) Why are we still using lead-free solder again? So it goes....
Joe
"Davide de Maio of National Physical Laboratory discussed the high frequency vibration testing of tin-lead and lead-free solder joints, with reference to automotive and aerospace electronics--a grim reminder that 80% of failures in airborne electronics were attributable to vibration and shock. A test piece had been designed representing a single solder joint between two copper components, which was tested to failure at frequencies of 400Hz and 800Hz. A range of SAC lead-free solders had been evaluated, with tin-lead as a comparison.
The tin-lead solder outperformed the lead-free examples, especially at the higher frequency. In general, failure occurred at or near the intermetallic interface, which would be expected to be the most stressed area. Of the SAC alloys, performance at 400Hz was better the higher the silver content. Annealing of SAC had a deleterious effect on performance at both 400Hz and 800Hz."
**************Make your life easier with all your friends, email, and favorite sites in one place. Try it now.
(http://www.aol.com/?optin=new-dp&icid=aolcom40vanity&ncid=emlcntaolcom00000010)
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
==============================================================================
This email and any attachments thereto may contain private, confidential, and privileged material for the sole use of the intended recipient. Any review, copying, or distribution of this email (or any attachments thereto) by others is strictly prohibited.
If you are not the intended recipient, please contact [log in to unmask]
immediately and permanently delete the original and any copies of this email and any attachments thereto.
==============================================================================
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|