Solder finish has been HASL and also seen with "tinned and fused".
Solder wets to the pads AND there is evidence the ball reflows.
The ball is pushed against reflowed solder on the pad to point it's out of
shape
(water balloon to solder mound).
Defect is not always on the corner pad, but can be the 2nd, 3rd or 4th in
from corner.
Thru destructive analysis have seen at least one example of farther in under
the package (in 5 rows).
RKUBES
-----Original Message-----
From: Earl Moon [mailto:[log in to unmask]]
Sent: Wednesday, November 15, 2000 8:52 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Soldering Problem
Are you soldering to gold pads? If so, have you checked for the black
plague?
Earl Moon
----------------------------------------------------------------------------
-----
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
----------------------------------------------------------------------------
-----
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|