Hi Gary,
2) Liquidous temperature, 183 oC for leaded and 217 oC for lead-free.
What you write is incorrect. 183C and 217C are NOT the Liquidus temperatures fro SNPb and SAC solders, respectively; they are their Solidus temperatures.
For eutectic SnPb the Liquidus and Solidus temperatures are the same, but for non-eutectic SnPb solders the Liquidus temperatures are higher. Eutectic SAC solder is not used—thus, any of the SAC solders have Liquidus temperatures higher than 217C. Thus, L(SAC405)=222C, L(SAC305)=220C,L(SAC205)=223C,L(SAC105)=226C, etc.
You need to reflow above the Liquidus not the Solidus temperatures.
Werner
-----Original Message-----
From: David D. Hillman <[log in to unmask]>
To: [log in to unmask]
Sent: Fri, Jun 26, 2009 2:59 pm
Subject: Re: [LF] Reflow profiles for mixed Pb status boards
Hi Gary - a couple of comments: (1) IPC -JSTD-002 is a solderability test
specification and is not relevant to your reflow questions in terms of
temperature range; (2) You will find there a two industry camps - the
camp that says "don't subject" tin/lead components to a leadfree reflow
profile because the components are not qualified for that process exposure
and the camp that says "do subject" tin/lead components to a leadfree
reflow profile but keep the temperature exposure as limited as possible in
terms of maximum temperature and duration. A product design team, in
conjunction with the component engineering team, need to determine if the=2
0
Camp 2 option is viable for their product. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Gary Koven <[log in to unmask]>
Sent by: Leadfree <[log in to unmask]>
06/26/2009 11:08 AM
Please respond to
"(Leadfree Electronics Assembly Forum)" <[log in to unmask]>; Please respond
to
Gary Koven <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[LF] Reflow profiles for mixed Pb status boards
For those of you who subscribe to the IPC DesignerCouncil email forum,
this will be a duplicate topic...
We have a number of PCBAs with both leaded and lead-free parts on them.
Looking over the J-STD-020 reflow profiles on one of the leaded part
datasheets, we saw that its range seemed too restrictive for the lead-free
profile.
Basically the two parameters that interest us are:
(1) Preheat temperature, 100 oC-150 oC for leaded and 150 oC-200 oC for
lead-free
(2) Liquidous temperature, 183 oC for leaded and 217 oC for lead-free.
On our assembly drawings we call out IPC-A-610 Class 2. I understand that
J-STD-002 can also be used together with IPC-A-610 as a note callout.
Since there is not a RoHS-compliant requirement for these boards, we don't
call out what type of solder process needs to be used.
We're curious about how assembly shops adjust their soldering process for
boards that have both types of parts on them.
We're also wondering whether we need to begin calling out specific solder
processes, but we don't want to add cost to the assem
bly.
Give me a solution that doesn't add cost to the assembly, but at the same
time satisfies the curious, please.
TIA and Best Regards,
Gary M. Koven, C.I.D.
Dynazign, Inc.
Charlotte, NC, USA
Veteran of the Marsh School
-------------------------------------------------------------------------------Leadfee
Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send:
SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-------------------------------------------------------------------------------
-------------------------------------------------------------------------------Leadfee
Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send: SET
Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-------------------------------------------------------------------------------
-------------------------------------------------------------------------------Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-------------------------------------------------------------------------------
|