Michael:
I'm NOT sure what Japan is doing, but:
Building MLBs w/o Lead can be accomplished by several means, it just
depends on what your assembly process can tolerate.
Typical finishes include:
Cu/Ni (Bright-Sulfate, or Matt Finish-Sulfamate)
Cu/Ni/Au (Electrolytic / Electroless / Immersion Au)
(w/ SOFT & HARD Gold options on Electrolytic)
Cu/Ni/Sn (Used this process in a past life )
OSP (this option typically sees Sn/Pb used as an etch
resist, but the finish composite contains none)
Gary Erickson
Hadco TechCenterEast
______________________________ Reply Separator _________________________________
Subject: Re: [LF] IPC Session on the "Problems and Promise of Lead
Author: Michael Meltzer <[log in to unmask]> at smtplink-hadco
Date: 7/7/99 10:10 AM
Chris,
Thank you for this information. I do have a question you might be able to
answer. I have read that Japan's Nortel has built a lead-free telephone.
This means that the phone's PC boards have no lead in them. Do you know
what they use in the place of HASL and Sn/Pb etch resists?
Thanks,
Michael Meltzer
Pollution Prevention Group
Lawrence Livermore Nat'l Lab
>Michael,
>
>I will make sure you are added to our distribution list for the final
>program we will
>be sending out within the next week or so. In the meantime, I would
>suggest you check
>the information we have posted on the IPC web site
>(http://www.ipc.org/html/ipcworks99.htm).
>
>You can also download the registration form
>(http://www.ipc.org/html/IPCWorksreg.pdf)
>from our web site.
>
>We will be opening a new web site dedicated to the issue of lead elimination
>(www.leadfree.org), and we have a free e-mail forum ([log in to unmask]) you
>can use to
>stay current on lead elimination.
>
>Using the e-mail forum, you can get the latest information on the
>conference and
>interact with your peers on lead elimination. Instructions for subscribing
>to the
>forum are included below.
>
>Please feel free to contact me directly with any further questions or
>concerns.
>
>Best regards,
>
>
>
>Chris Jorgensen
>Technical Project Manager
>IPCWorks '99 Conference Coordinator
>
>An International Summit on Lead-Free Electronics Assemblies
>October 25 - 28, 1999
>Hyatt Regency, Minneapolis, MN
>
>To stay on top of the lead elimination issue, subscribe to the
>[log in to unmask]
>e-mail forum.
>
>To subscribe compose the following email message:
>TO: [log in to unmask]
>SUBJECT: (leave blank)
>MESSAGE: subscribe leadfree YOUR NAME
>
>
>>>> Michael Meltzer <[log in to unmask]> 07/06/99 06:37PM >>>
>I'm very interested in attending. My name and data are:
>
>Michael Meltzer
>Lawrence Livermore National Laboratory
>PO Box 808, L-633
>Livermore CA 94551
>(925) 424-6923
>[log in to unmask]
>
>
>>Dear Leadfree Subscribers:
>>
>>The IPC is hosting an international summit on lead-free electronic
>>assemblies from October 23-28 in Minneapolis, Minnesota. At the summit,
>>the Environmental, Health, and Safety Committee of the IPC will hold a
>>session on Monday, October 25th from 9 AM to noon, entitled: "The Problems
>>and Promise of Lead in Electronics."
>>
>>The session is designed to help illuminate the public policy debate over
>>the continued use of leaded solders in the electronic industry, focusing on
>>the environmental risks posed by leaded solders and the environmental risks
>>posed by possible alternatives. It is designed to help members understand
>>both the fact and fiction behind the debate so that members can voluntarily
>>decide which solders will work best for their own particular applications.
>>
>>As you may know, the European Union is proposing to ban the use of lead in
>>electronic devices by the year 2004 due to concerns that, when disposed of,
>>electronic devices will leach lead into groundwater. However, some industry
>>representatives contend that such concerns are unwarranted or could be
>>addressed through other policy options, such as increased recycling.
>>Futhermore, there is concern that alternatives to leaded solders could pose
>>other environmental problems.
>>
>>This session is designed to illuminate the issue so that participants can
>>better understand the environmental impacts associated with the industry's
>>continued use of leaded solders. The IPC is currently soliciting papers
>>for this session. Currently, the format of the session is very open.
>>Possible topics include:
>>
>>- the environmental risks posed by leaded solders in electronics
>>- the environmental risks/benefits of alternative solders
>>- policy options for reducing the environmental risks posed by leaded
>>solders (International, federal, or state)
>>- cost-benefit studies of leaded solders or their alternatives
>>- Life Cycle Analysis of leaded solders or their alternatives
>>
>>Again, the purpose of this panel will be to help clarify the science behind
>>this issue so that the IPC members become more aware of the environmental
>>risks associated with leaded solders and their alternatives.
>>
>>Please e-mail me directly if you are interested in participating in this
>>session.
>>
>>Sincerely,
>>
>>
>>
>>
>>Holly Evans
>>Director of Environmental and Safety Programs
>>IPC
>>2600 Virginia Ave., Suite 408
>>Washington, D.C. 20037
>>Phone: 202-333-2331
>>Fax: 202-333-6605
>>E-mail: [log in to unmask]
>>
>>################################################################
>>Leadfree E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>>################################################################
>>To subscribe/unsubscribe, send a message to [log in to unmask]
>>with following text in the body:
>>To subscribe: SUBSCRIBE Leadfree <your full name>
>>To unsubscribe: SIGNOFF Leadfree
>>################################################################
>>IPCWorks -October 25-28 featuring an International Summit on Lead-Free
>>Electronic
>>Assemblies.
>>Please visit IPC's Center for Lead-Free Electronics Assembly
>>(http://www.ipc.org/html/leadfree.htm ) for additional information.
>>For technical support contact Gayatri Sardeshpande [log in to unmask] or
>>847-790-5365.
>>################################################################
>
>################################################################
>Leadfree E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask]
>with following text in the body:
>To subscribe: SUBSCRIBE Leadfree <your full name>
>To unsubscribe: SIGNOFF Leadfree
>################################################################
>IPCWorks -October 25-28 featuring an International Summit on Lead-Free
>Electronic
>Assemblies.
>Please visit IPC's Center for Lead-Free Electronics Assembly
>(http://www.ipc.org/html/leadfree.htm ) for additional information.
>For technical support contact Gayatri Sardeshpande [log in to unmask] or
>847-790-5365.
>################################################################
>
>################################################################
>Leadfree E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask]
>with following text in the body:
>To subscribe: SUBSCRIBE Leadfree <your full name>
>To unsubscribe: SIGNOFF Leadfree
>################################################################
>IPCWorks -October 25-28 featuring an International Summit on Lead-Free
>Electronic
>Assemblies.
>Please visit IPC's Center for Lead-Free Electronics Assembly
>(http://www.ipc.org/html/leadfree.htm ) for additional information.
>For technical support contact Gayatri Sardeshpande [log in to unmask] or
>847-790-5365.
>################################################################
################################################################
Leadfree E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask]
with following text in the body:
To subscribe: SUBSCRIBE Leadfree <your full name>
To unsubscribe: SIGNOFF Leadfree
################################################################
IPCWorks -October 25-28 featuring an International Summit on Lead-Free
Electronic
Assemblies.
Please visit IPC's Center for Lead-Free Electronics Assembly
(http://www.ipc.org/html/leadfree.htm ) for additional information.
For technical support contact Gayatri Sardeshpande [log in to unmask] or
847-790-5365.
################################################################
################################################################
Leadfree E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask]
with following text in the body:
To subscribe: SUBSCRIBE Leadfree <your full name>
To unsubscribe: SIGNOFF Leadfree
################################################################
IPCWorks -October 25-28 featuring an International Summit on Lead-Free Electronic
Assemblies.
Please visit IPC's Center for Lead-Free Electronics Assembly
(http://www.ipc.org/html/leadfree.htm ) for additional information.
For technical support contact Gayatri Sardeshpande [log in to unmask] or 847-790-5365.
################################################################
|